含镉银钎料主要技术参数 Technical Characteristics of silver alloys with cadmium: |
钎料牌号 Brazing Alloys |
主要化学成份 (%) Chemical Composition |
熔化温度℃ Melting range ℃ |
焊接温度℃ Working temperture℃ |
强度(N/mm) Trensile |
相当于其它 标准牌号 Ref. code in other standards |
公司代号 Huazhong code |
Б |
t |
BAg5CuZnCd |
Ag:5;Cu:53; Zn:35;Cd:7 |
770~820℃ |
820~920℃ |
/ |
/ |
|
HY051A |
BAg10CuZnCd |
Ag:10;Cu:48; Zn:32;Cd:10 |
760~810℃ |
810~910℃ |
/ |
/ |
|
HY101A |
BAg12CuZnCd |
Ag:12;Cu:41;Zn:34; Cd:12;Sn:少量 |
750~800℃ |
800~900℃ |
/ |
/ |
|
HY121A |
BAg15CuZnCd |
Ag:15;Cu:42; Zn:28;Cd:15 |
745~800℃ |
800~880℃ |
/ |
/ |
|
HY151A |
BAg18CuZnCd |
Ag:18;Cu:38; Zn:27;Cd:17 |
740~780℃ |
790~880℃ |
310 |
25 |
|
HY181A |
BAg20CuZnCd |
Ag:20;Cu:40; Zn:25;Cd:15 |
705~780℃ |
800~870℃ |
305 |
30 |
|
HY201A |
BAg25CuZnCd |
Ag:25;Cu:31; Zn:27.5;Cd:16.5 |
680~780℃ |
780~850℃ |
290 |
30 |
|
HY251A |
BAg30CuZnCd |
Ag:30;Cu:28; Zn:22;Cd:20 |
650~750℃ |
740~840℃ |
300 |
30 |
China HL311 AWS BAg-2a |
HY301A |
BAg35CuZnCd |
Ag:35;Cu:26 Zn:21;Cd:18 |
605~700℃ |
700~845℃ |
300 |
30 |
China HL314 AWS BAg-2 |
HY351A |
BAg40CuZnCd |
Ag:40;Cu:19 Zn:21;Cd:20 |
595~605℃ |
605~705℃ |
300 |
30 |
China HL312 AWS BAg-4 |
HY401A |
|
BAg40CuZnCdNi |
Ag:40;Cu:16;Zn:18; Cd:26;Ni:少量 |
595~605℃ |
605~705℃ |
300 |
30 |
|
HY401A+ |
BAg45CuZnCd |
Ag:45;Cu:15; Zn:16;Cd:24 |
690~620℃ |
620~760℃ |
300 |
30 |
AWS BAg-1 |
HY451A |
BAg50CuZnCd |
Ag:50;Cu:15; Zn:17;Cd:18 |
625~635℃ |
635~760℃ |
340 |
30 |
China HL313 AWS BAg-1a |
HY501A |
BAg50CuZnCdNi |
Ag:50;Cu:16;Zn:15 Cd:16;Ni:3 |
630~690℃ |
690~815℃ |
350 |
35 |
AWS BAg-3 |
HY501A+ |
应用说明 Applications |
· 此类银钎料用于钎焊绝大多数黑色金属和除铝与镁及其它低熔点金属以外的所有有色金属。这类钎料具有良好的钎焊性能可以使用所有的加热方法,但除真空或保护气氛中钎焊以外,通常需要配用钎剂; · 为降低熔点及减少白银含量,加入镉、锡、镍等构成三元或多元合金钎料,此类钎料因含有镉,具有一定的毒性,达不到欧盟ROSH标准要求,不适宜于与食物、饮用水直接接触接头的钎焊; · 钎焊前必须严格清除钎焊表面的油脂、氧化物等污物,钎焊接头最好间隙为0.03~0.075mm。 |