/*%3C%21%5BCDATA%5B*/var%20hash%3Dwindow.location.hash.match%28/%5E%23sub%28%5Cd+%29/%29%2ClemmaHashFound%3Dfalse%3Bbk.view.hash%3Dhash%26%26hash%5B1%5D%3Bhash%3Dnull%3Bif%28bk.view.hash%29%7Bvar%20lemmaDescArray%3D%5B%7B%22subLemmaId%22%3A3423370%2C%22subLemmaDesc%22%3A%22W302%22%7D%5D%3Bbaidu.array.each%28lemmaDescArray%2Cfunction%28_%2CA%29%7Bif%28bk.view.hash%3D%3D_.subLemmaId%29%7BlemmaHashFound%3Dtrue%3B%7D%7D%29%3B%7D/*%5D%5D%3E*/
bk.view.expFlag%3Dfalse%3BbaikeViewInfo%3D%7Bid%3A%223423370%22%2Ceditable%3A%22true%22%2Ctitle%3A%22W302%22%2CexpIndex%3A%220%22%2CsubLen%3A%221%22%2CisMulit%3Afalse%2CsubList%3A%5B%7B%22subLemmaId%22%3A3423370%2C%22subLemmaDesc%22%3A%22W302%22%7D%5D%7D%3B
W302 奥国“百禄”热作模具钢。出厂状态: 退火最高硬度235HB. 钢材特点:具有高温耐磨性,
编辑本段
w302介绍 热强度高。抛光及切削容易,可表面氮化,火花机加工。用途:适合各种热作用途,如压铸模,热合金或金属挤压模,射咀,射筒,热剪刀,塑料模,等等。 出厂状态:软性回炉至HB235(最高)
特性应用:钢质洁净均匀,结构良好,用3000-6000吨压
横锻压,冲击强度高,经超声波检验,材料利用率高,且可减少加工费用,有最佳之红热硬度,韧性高强.可制
锌\铝\铅\锡等合金或铜合金之压铸模,唧咀,挤压轴心等,可用作热锤或热冲铸模,经淬硬后可作永久性生产塑胶模
编辑本段
热处理工艺 锻制:1100℃开始锻打至900℃回炉随炉冷却
退火:750—800℃保温后炉冷却,可达硬度235HB(最高)。
淬火:由1020—1080℃油或空冷,必须将至60—80℃即时回火。
回火:第一次火约500℃以获得第二次硬化之最高硬度;第二次回火等于500℃以达到所需硬度;第三次回火温度稍低於前者温度(约30℃)。
编辑本段
w302化学成分 C碳 0.40,Cr铬 5.00,
Mn锰 0.40,
Mo钼 1.30,
V钒 1.10,
Si硅 1.00