供应化妆品瓶盖专用PCTG AN011 高透明 耐化学PCTG
Regular Transmittance
89%
Product Data Sheet
Eastar™ Copolyester AN011, Natural
|
| Application/Uses | - Cosmetics/personal care packaging
- Fragrance packaging
|
| |
|
| Product Description |
| Eastar™ AN011 copolyester is a high flow product. Eastar™ AN011 flow lengths are increased 20-40% relative to Eastar™ AN001 as shown by spiral flow testing. Other outstanding features of Eastar™ are easily maintained such as excellent appearance and clarity, good physical properties, chemical resistance, and easy processing. This high flow product is especially suited for those applications utilizing thin-walled intricate tools. Under existing United States Food and Drug Administration (FDA) regulations, Eastar™ AN011 may be used in food contact articles which comply with the specifications and conditions of use in 21 CFR 177.1240. This product has been GREENGUARD INDOOR AIR QUALITY CERTIFIED®. The GREENGUARD INDOOR AIR QUALITY CERTIFIED® Mark is a registered certification mark used under license through the GREENGUARD Environmental Institute (GEI). GEI is an industry-independent, non-profit organization that oversees the GREENGUARD Certification Program. The GREENGUARD Certification Program is an industry independent, third-party testing program for low-emitting products and materials for indoor environments. For more information about GEI and to obtain printable certificates for Eastman™ Copolyesters, visitwww.greenguard.org. Choose Eastman Chemical Company under the Manufacturer category and click search to display a list of our products. |
|
| Typical Properties |
| |
| |
| Propertya | Testb Method | Typical Value, Unitsc |
| |
| General Properties |
| Specific Gravity | D 792 | 1.19 |
| Mold Shrinkage | D 955 | 0.003 mm/mm (0.003 in./in.) |
| Water Absorption, 24 h immersion | D 570 | 0.15% |
| |
| Mechanical Properties |
| Tensile Stress @ Yield | D 638 | 50 MPa (7200 psi) |
| Tensile Stress @ Break | D 638 | 43 MPa (6300 psi) |
| Elongation @ Yield | D 638 | 5% |
| Elongation @ Break | D 638 | 270% |
| Flexural Yield Strength | D 790 | 68 MPa (9800 psi) |
| Flexural Modulus | D 790 | 1900 MPa (2.7 x 105 psi ) |
| Rockwell Hardness, R Scale | D 785 | 107 |
| Izod Impact Strength, Notched |
| D 256 | 80 J/m (1.5 ft·lbf/in.) |
| D 256 | 44 J/m (0.8 ft·lbf/in.) |
| Impact Strength, Unnotched |
| D 4812 | NB |
| D 4812 | NB |
| Impact Resistance (Puncture), Energy @ Max. Load |
| D 3763 | 40 J (30 ft·lbf) |
| D 3763 | 38 J (28 ft·lbf) |
| |
| Thermal Properties |
| Deflection Temperature |
| D 648 | 73°C (163°F) |
| D 648 | 66°C (150°F) |
| Vicat Softening Temperature @ 1 kg load | D 1525 | 86°C (186°F) |
| |
| Optical Properties |
| Total Transmittance | D 1003 | 92% |
| Haze | D 1003 | < 1% |
| |
| Typical Processing Conditions |
| Drying Temperature | | 70°C (160°F) |
| Drying Time | | 4 hrs |
| Processing Melt Temperature | | 230-280°C (450-530°F) |
| Mold Temperature | | 15-30°C (60-80°F) |